Part is 1/2 blue 4A, 1/2 Deep red. red fades when boiled
Product: anodize
Base Metal: Aluminum
Amperage: 5
Voltage: 13
Temperature: 75
Duration: 100
Area: 140
Power Source: batt charger
Surface Prep: Buff,soap,desmut,rinse
Problem: Part is 1/2 blue dye 4A and 1/2 Deep red. When the part hits the boiling water for sealing the blue looks great and the red fades FAST and comes of in areas. BOTH BLUE AND RED LOOK GREAT until the part hits the water.
Solution:
Try hanging the part in the STEAM for 15 mins prior to immersion. Failing that, post this on the forum. There could be several things wrong here, and you'll get several answers.
Comment/Problem: Yes this was better but the red dye bled onto an area that was suppose to be silver and still got streaks from the steam. Is this just a problem with red dye and boiling or am i making a mistake with anodizing times ?
|