View Single Post
  #3 (permalink)  
Old 07-27-2004, 08:24 PM
clab clab is offline
Newbie
 
Join Date: Jul 2004
Location: Floyd, VA
Posts: 6
clab
Default Strip the tin first

I got not so good results going over the tin/solder plate on my pcbs. I tried a number of strip methods (mechanical) and none really worked well enough. I found that nitric acid diluted with a bit of 12% hydrogen peroxide applied with a Q tip worked well for this. Then nickel, then gold, and it's as good as the pros can do it.
Reply With Quote