i used that chromex ... it is sweet and cheape... i would say if you want a nice chrome look use it .... a compressor and a detail spray gun and don't use glass bead it dose not stick i found that out the hard way ...
here is what i do :
1. clean and degrease
2. i blast it with sand ( it is a healt risk but it makes it bond good)
3. wipe down with thinner
4. spray at 32 psi ( must use filters to tram any water or oil caswell stocks them)
5. i bake it at 500 f for 1 hour
6. polish with 0000 super fine steel wool
7. glass bead at 25 psi and it looks better than chrome plate
|