Re: Anyone use the Iron Phosphate Primer?
I usualy spray it on for around 2-3 min then spray it down with water put it in the oven at low temp to help dry then powder and bake. works great. you dont want to leave it on too long or it will start to oxidize. around a couple of min then wash off with clean water. that stops the reaction. and dont touch with your hands, it leaves a crystal like sturcture on the parts and if you touch it the oils from your hands will cause it to break down. i use a rolling rack that i can phosphate then wash then roll into the oven i never have to touch the parts till done.
Joe
|