This is the write up I promised back around Christmas but due to family issues I was not able to get to it...
The 2 Images attached are done with extreme chrome and super high gloss clear coat.
Image 0504 is just Chrome:
Image 0506 has teh clear coat on it..
Now the How To Part of this post..
Do your prep as normal,
Apply Chrome as normal BUT applying only enought to coat and not over coat you want a good thin layer. Now Cure at 375 for 30 mins, yes this is after it has come up to that temp ( the part not the oven ).
After curing let part(s) cool to room temp this is very important that it is room temp!!!
Now reheat part to 150 degree's +/- 10% remove from oven then clear coat for the required time, No more no less.
So far I have used over a pound of powder each and have turned out the same results each and ever time.. With very very little to no cloud effect..


Jim S...
Attached Thumbnails
extreme-chrome-clear-coat-how-0504.jpg  extreme-chrome-clear-coat-how-0506.jpg  
__________________
Jim Shuster
www.backyardpowdercoating.com Sold.....
www.chrissys68mustang.com Hobbie
www.photogserver.net Web Hosting.
Reply With Quote