I just recentily started annodizing ( 3 days ago)
The results have been pretty good sofar, but it never reaches par.
Example: I did one of the test bars(completly submersed) total Surface Area-21.375 in.
According to the 720 rule @4.5 amp/sq ft thats .67 amp, 96 min with a par of 11.25V.
My voltage went slowly from 8.9 to 8.6 and the bar dyed nicely.
http://www.flickr.com/photos/yoyoboy/102796525/
Another Example: A yoyo I did total SA of 34.143 sq in @ 6 amp/sq ft and .8 mils
Gives us 1.42 amp, for 96 min and a par of 15 volts.
My voltage looks this:
Time Remaining Volts
1:36 18.3
1:10 18.1
50 17.9~17.8
46 17.5
Then It jumps and stays relatively steady( I wasnt there for thease 10 min)
36 21.8
33 21.5
28 21.5
21 21.2
15 20.9
3 20.5
0 20.4 And I contuied to run the part for another 20 min with the voltage staying the same.
Taking a look at the part You will notice the the unannodized patches. I'm thinking they are caused by insufficient cathodes( 1 GP plate) But why is the voltage so high?
Ignore the crappy masking job
http://www.flickr.com/photos/yoyoboy/102796525/
EDIT: maybe you cant see the bare spots.
So, What's causing the high/low voltage? and the bare spots?