View Single Post
  #3 (permalink)  
Old 02-21-2006, 11:56 PM
yoyoboy yoyoboy is offline
Newbie
 
Join Date: Nov 2005
Posts: 31
yoyoboy is on a distinguished road
Default Re: So I've done a few runs and am starting to have problems..

UPDATE:
Well actually I didnt want to put it all in one post.
So I did my Ego(paintball gun) And had a lot more problems.

I did half of the parts, because they would not all fit into my tank. Infact I think some of the problems might be caused by over crowding in the tank.

163" .75 mils 4.5amp/sq ft.
gives 5.1 amps for 120 mins with a PAR of 11.25
Time-voltage looks like this:
2:00 5.9
1:42 6.3
1:30 6.3
1:17 6.3
1:04 6.3
43 6.4
34 6.5
15 6.8
10 7.0
6 7.1
0 7.2
I then ran it for 5 more mins and it stayed at 7.2
The body and on/off took dye, but the grip frame , the barrel back, and the other parts didnt.
What they did do is have little speckles of dye on them. I am thinking that thease may have been because of there placement in the tank prevented them form getting areation and the hydrogen bubles built up. Also some of the parts where above the cathode level- (I got lead flashing and now having it running all the way around the sides, but it doesnt go all the way up)
I assume the blotchyness on the body is caused by how it was dyed( I was a bit more concerned with the parts that wernt dying at the time, and wans't verry carfuel while handiling it.
The way I dyed it was on a metal screen with wood runing around the sides.

So whats causing the the Spots? And why did some parts not dye? HELP!