Default Re: battery acid mixture

A 1:3 ratio (battery electrolyte : distilled water) is the correct ratio for LCD anodizing. It will work for CD's up to 12A per square foot. A 1:2 or 1:1 ratio is for higher amperage anodizing or used in the past by many using the let it rip method. Using them below a 12A CD will cause dissolution problems among others.