Re: Safe process for pot metal and aluminum?
Is it just the copy chrome that your tring to use, or all three plating steps
(copper,nickel,chrome)
If you can get the copper on the parts from a bath, then I know you can nickle and chrome the parts. I use to do the brush plating...your going to need the flash copper for pot-metal or alum. its easier than the nickle strike. If the parts react with muratic then its pot-metal, you want to mix 50/50 muratic and water for your pot-metal etch, then go into your flash copper..of course this is after your proper prep of the parts.
|