70 Degree temp.
Ecthed parts lye for 3 min.s Parts began to bubble like "aklaseltzer in coca-cola" Removed parts and rinsed in distilled water
Placed parts in acid solution, turned on power
SA 23.385 IN sq
Set amps to .73 as per 720 rule, parts bubbling like crazy
Starting voltage was 5 volts, never got 11.25 volts as per 720 rule
At 40 min.s voltage was 5.4 volts
At 45 min.s voltage was 7.2 volts
At 50 min.s - 7.7 volts
At 58 min.s voltage shot up to 18.4 volts, amps dropped to .61
At 1 hour 10 min.s part #2 is the only one still bubbling (rest stopped)
At 1 hour 12 mins, Amps dropped to .13 - Volts stayed 18.4V
Removed parts and rinsed.

RESULTS - Part 1 & 3 Barely took color
Part 2 came out a dark pinkish rose color w/ red small lines (Looks almost like cracks, but are not, just looks that way)
Reran part no, 1, by itself, came out slightly darker, but not as dark as part no. 2
any help would be apprieciated , Thanks