Quote:
|
Originally Posted by cruizer
The problem I have with taping off areas is it ususaly leaves a not so nice edge. Ussally a rogh edge that looks like I taped, painted, and then pealed it off. I mean it's not a nice edge. Does anyone else have this problem?
|
Cruizer,
Here is the secrete to taping. Mask your area, powder pre-bake just until the powder starts to melt then remove from oven let cool so you can remove the tape. Place back in oven for full cure..
This will remove all those rough edges..
Jim S...