Prep how ever you like. But here are my steps..
1. Sand Blast parts to remove old coating.
2. Wipe done with acetone. Do not touch with bare hands from this point on.
3. If used parts you may want to outgas at 450 degrees for 30 mins ( time starts once part reach's 450 degrees)
4. If Out gassed let part reach 150 degrees, if New part and no out gassing go a head and shoot powder at room temp.
5. Place part in cool oven set temp to 392 degrees for Extreme Chrome. Once part rreach's 392 degrees start timer for 15 mins.
6 Remove from oven let part cool to room temp.
7. Rewarm part to 150-170 degrees.
8. Shoot candy color onto part ( Remember DO NOT TOUCH PART WITH BARE HANDS).
9. Cure part at 400 degrees for 10 mins. The time starts once the part reach's 400 degrees.
10. Let cool in oven by cracking door open.
11. Enjoy new candy color and ship to client...

Remember all times start once the part reach's Cure temp, this is why you need a Lazer temp guage.
I have shot just about ever candy color out there and these are my steps.. Work ever time...