View Single Post
  #6 (permalink)  
Old 07-24-2006, 09:04 PM
acidrain acidrain is offline
Metal Finishing Guru
 
Join Date: Sep 2004
Posts: 881
acidrain is on a distinguished road
Default Re: fingerprinting issues on anodized alum.

What alloy, CD, tank temp, and sealing process are you currently using?
It could be desolution... is the surface chalky?
It could be lack of thorough sealing... are you steam sealing, or using the nickel acetate high temp sealer?
I use the nickel sealer at near boiling temp for 20min for .75mil, and 30min for 1mil ano thickness.
__________________
Specializing in anodized graphics in Paintball guns.