Try reducing the rubber cement with lacquer thinner... it will make it less stringy. You may have to give it a couple coats though.
Also, after you bleach the area, rinse well, then dip in 1:3 sulfuric acid/water, then rinse again. That will help remove any remaining dye, and will also liberate any remaining chlorine in the pores so the next color will take.