That will work for up to about .5 sq. ft of surface area.
For sure get all your chemicals from caswell. Don't bother with the rit dye.. get real ano dye.
For new parts, all you will need is SP degreaser, dye, and high temp sealer.
If the parts are oxidized, or for stripping and re-anodizing older parts, you'll need stripper/etch, and desmut/de-ox.
Stripper/etch at room temperauture, desmut/de-ox at 120-140F, SP degreaser at 140F, ano tank at 68-70F, dye at 140F, and seal at over 180F.