Re: LCD method
My air source is actually my big industrial air compressor with a good in-line filter. I built a CPVC manifold with 1/16in holes drilled every 4in or so. I regulate the air down to about 20psi line pressure, then regulate it again at the tank to control the bubbles.
I run at 6 amps CD... there are advantages to LCD: low heat accumulation, low fumes, good color absorbtion, and clear parts come out silver... not yellow.
I try to stay at least 3 inches away from the cathode.
GL!
__________________
Specializing in anodized graphics in Paintball guns.
|