I have been finding out also that the temp. of the copy cad electrolyte plays a big roll in the process, when i go above 90 degree,s it seems like all my parts go grey color on me, if i let the temp drop to 80 it makes a world of differance. Also i have been experimenting with my circulating pump, it also makes a differance, if its not moving the electrolyte around well, parts don,t want to plate.Remember i know its a pain but the better the parts are degreased and polished the better they come out, small parts to me are a pain,patience is the no.1 cure.