Reduce by ~25%

5xxx and 6xxx alloys (@6ASF)
.5 mil - gold, clear, light colors 1 hr
.75 mil - medium colors like blue, orange, etc 1 h 30 m
1 mil - red and black 2 hr

2xxx and 7xxx alloys (@6ASF)
.5 mil 45 min
.75 mil 1 hr 12 m
1 mil 1 hr 30 min

theres ya some run times.

I often run all alloys together and just take the 2x and 7x out when there time is up.This does not work every time.It can cause the ps to jump and possibly cause the parts to lose connection.You also have to have the the sq area of the parts left in the tank that way you know how much to turn the amperage down.