fill the cup up maybe 1/2 way. if it's too full, you'll get clouds.

also, when you remove the cup and look at the little nub sticking up (fluidizer), it has a hole in it. air flows through that hole to stir up (fluidize) the powder. drill 2 or three more holes of the same size in the nub. this will improve fluidization and reduce the puffs of heavy powder.

aslo shake the powder before shooting to loosen it up.