Default Re: How do you powder coat two different colors with a nice sharp edge

Shoot the letter color first and bake. Mask the letters using high temp tape then shoot the background color. Bake just long enough to set the background color (so you don't knock it off), cool then remove the tape. Return it to the oven and complete the bake. This is reverse of how the plate was painted but it's easier to use the width of the tape as the letters than trying to mask the background.