amobine, ive been using my copy cad system for about a yr. now, every part comes out almost as perfect as i want, i glassbead part,degrease part, then simply polish it up on a wire wheel that i have mounted on my workbench,parts coming out awesome, is this the same prodecure you are using, most carb. parts are cad. plated at 1.5 amps and .7 volts and 90 degree,s, i still don,t like the 110 degree temp. but 90 works great for me. parts are put into a mauratic acid bath for 8 to 10 sec. then washed off with distilled water, then into the electrlite bath for about 8 to 10 min., parts come out awsome for me. Please post a picture of your set-up and maybe we can help you out. e-mail me anytime for help and ill see what i can come up with, ok