View Single Post
  #7 (permalink)  
Old 06-04-2008, 11:17 AM
seanc seanc is offline
Zinc Plating Guru
 
Join Date: Jun 2003
Posts: 321
seanc is on a distinguished road
Default Re: Fresh copy cad system leaving white swirls

Odd. I've been told the range is 90-120º, w/100-110º optimum.

Sounds like after step 7, it's just raw zinc? No chromating?

How are they being dried? Drip-dry, warm air, hot air, oven?

Again, sounds to me like accelerated oxidation.

If the parts are NOT chromated, you might try spraying w/WD-40 after final rinse, then let that drip-dry for a day.

Sean
__________________
Seans Zinc Plating page