Default Re: Fresh copy cad system leaving white swirls

Quote:
Originally Posted by MrPontiac View Post
.. ive never read anywhere to where it says dry with hot air
Well, it doesn't say that anywhere for the electrolyte, but can be helpful. It DOES say "best hot air dryed @ 150º" for the chromates, and it's useful to prevent water stains. You can't get it TOO hot though.

So again, are you chromating?

Quote:
Oh, yes with the 40 min plating time im loosing all gloss on parts
Time should not be an issue. Are you using the "brightener"? Perhaps that's been depleted.

How big are these "rear plates"?

Sean