Originally Posted by benherr View Post
Mikmj,
I'm using the super wet Black. This morning I did another PC. Yesterday I cleaned the oven with Easy-off. Preheated oven to 400deg. Sanded the piece down to smooth, cleaned twice with acetone and then applied a mist of LiquiguardPC (from Caswell for aluminum) applied the powder not too thick and not too thin. Placed in oven, waited till piece reached 392 degs. per the can and let set for 10 minutes and removed piece. Had lots of carters and minimual OP. this is starting to drive me rat s**t.

Ben

PS I do use a IR temp gun




Lose the LiquiguardPC and dont use acetone to wipe down powder it can turn it soft use alcohol. LiquiguardPC will cause crators too..............
__________________