Thumbs up Re: 24k gold plating kit

Hello,
If you want to plate on diecast:
1. Buff and polish diecast.
2. Copper strike- Copper under plate is your barrier to diecast.
3. Copper plate (100 microinches).
4. Buff/polish if you wish.
5. Clean/acid activate.
5. Plate nickel (100 microinches).
6. Activate acid dip.
7. Plate gold.
Good Luck,
NOL4154



hi ,i am new at this ,i want to gold plating diecast (hotwheels)in to gold but i thing i have to put nickel on it before.can someone give me a good trick or way to do this in a perfect way and what do i need for this.