Hello Again,

Thanks for your input fibergeek. I did try alum wire last night with great results. I also tried the titanium wire again. I bought some #10-24 alum screws and screwed each peice tightly to the tank bar and wire. I still had the titanium wire disolve at 55 mins into the anodizing process. the part was able to be dyed but a very thin layer. The alum part with the alumwire came out great. I had no problems with this and the color looked to be pretty even. I guess i didnt read the warning lable on the carton of battery acid that said will disolve titanium wire under mild aggitation. lol I would say I have come to a close with this problem and appreciate your input.
thanks again...
Cyber(Erik)