No it shouldn't chip off. It's either a cleaning problem or the nickle passivated before it went into the chrome. You should strip the chrome with pickle#2 muratic(hydrochloric) and the nickle with pickle#3 sulfuric. Pickle #3 will also activate the nickle. Read the manual for more details.