OK, here's what I do:
1 - De-grease with soft scrubb, rinse with distilled water.
2 - Sandblast the beegeebers out of it.
3 - quick rinse with distilled water to remove sand residue.
4 - flash-copper @.05adc for 1 minute, then @.03adc for 1 hour.
5 - remove from flash - rinse (distilled water) - acid copper for at least 1 hour at .03adc @75-80 degrees.
Good luck!