Hi All,

I live in the Caribbean and I’m setting up to do my first plating using Copy Chrome in a 15 gal tank. I got an Email from Tech Support to use it at 75 deg F. I suddenly realize it may get down to 75 deg F here in the morning, but most time of the day, especially during summer I would be dealing with 80-100 deg F.
I now wonder,
- Do I have to install air conditioning?
- Will I get away with it, using the Copy Chrome process at 80-100?
- Does anyone know an easy way to bring the temperature of tank down in this case?
Advice is much appreciated.

Stefan
Reply With Quote
  #2 (permalink)  
Old 02-02-2005, 07:56 PM
Moderator
 
Join Date: Feb 2003
Location: Texas
Posts: 269
dadkar2 is on a distinguished road
Default

I can't see why it wouldn't work at the elevated temperatures you're describing.

Ken
Reply With Quote
  #3 (permalink)  
Old 08-26-2005, 05:07 PM
jimcarry's Avatar
Experienced Metal Finisher
 
Join Date: Jul 2004
Location: Arkansas
Posts: 370
jimcarry is on a distinguished road
Send a message via Yahoo to jimcarry
Default Re: Temperature for Copy Chrome

I have been using Copy Chrome for a year here with great results when I first started I tried to plate at just 75 but I found that the Copy Chrome works best at 95-110 with lower amps the book says 1 amp per 16sq” but I usually cut this in half and plate for a longer time for instance if it says 1 hour I plate for 1.5 hours
__________________
Jim Eaton
Reply With Quote
Reply

Bookmarks


Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
 
Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off

Similar Threads
Thread Thread Starter Forum Replies Last Post
copy chrome vs triple chrome plating splbnd27 Electroplating Questions 18 06-21-2006 08:35 AM
Copy Chrome Start-up Elitefisherman Electroplating Questions 10 04-18-2004 05:24 AM
Copy Chrome Questions junodale Electroplating Questions 13 03-17-2004 12:15 PM
Chrome (re)plating question - howto olaf_sc Electroplating Questions 1 07-29-2003 03:00 PM
Hard chrome vs triple chrome butters Electroplating Questions 1 02-20-2003 12:35 AM


All times are GMT -4. The time now is 09:38 PM.


Powered by vBulletin® Version 3.7.4
Copyright ©2000 - 2008, Jelsoft Enterprises Ltd.
Search Engine Friendly URLs by vBSEO 3.2.0
Copyright © Caswell Inc.