Default Re: Cast iron in zinc

eprigge,

This could very well be and would be nice to fix since I've got 3 buckets full of old bath that is currently unusable. Problem is I can't find a good PH tester to save my life. My dad let me borrow one from his swimming pool kit but it only tests within a narrow range. I'll check with Cas tech support.

K-
Reply With Quote
  #12 (permalink)  
Old 05-28-2006, 11:24 PM
sswee's Avatar
Moderator
 
Join Date: Nov 2004
Location: close to Austin, Texas
Posts: 1,229
sswee is a jewel in the roughsswee is a jewel in the roughsswee is a jewel in the roughsswee is a jewel in the rough
Default Re: Cast iron in zinc

Caswell offers a Digital PH meter.

http://www.caswellplating.com/kits/ph_tester.html

SS
Reply With Quote
Reply

Bookmarks


Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
 
Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off

Similar Threads
Thread Thread Starter Forum Replies Last Post
Flash rust on cast iron chromeitout Powder Coating Questions 2 04-11-2006 11:39 PM
Zinc Die Cast hademes Plating Pot Metal 2 04-25-2005 10:46 PM
Anybody ever polished a cast iron engine block? thesound Metal Polishing Questions 5 02-10-2005 11:31 AM
Prepping cast iron. Stytooner Powder Coating Questions 3 08-04-2004 10:30 AM
Cast iron prep ewmorritt Metal Polishing Questions 1 05-28-2003 01:31 AM


All times are GMT -4. The time now is 04:07 PM.


Powered by vBulletin® Version 3.7.4
Copyright ©2000 - 2008, Jelsoft Enterprises Ltd.
Search Engine Friendly URLs by vBSEO 3.2.0
Copyright © Caswell Inc.