Default Yellow Chromate & Copy Cad

Hi. I had the kit for about three weeks now, it is still awesome. Have absolutely no complaints, praise only. However, I was under an impression that Yellow Chromate will dye even commercially obtained zinc plated items. I tried to "yellow" some nuts and bolts from a local hardware store, the color seems to be right, but the yellow finish can be rubbed off with a shop towel (24 hours later)! The items were properly degreased and I tried some battery acid on them, zinc reacted very rapidly. What am I doing wrong? I must note that my freshly plated parts accept Chromate well and finish seems somewhat durable, still VERY easy to remove the yellow coloring with steel wool. My chromate solution is applied for two minutes at 22 deg. Cel. Thanks.
Andrew.
Digg this Post!Add Post to del.icio.usBookmark Post in TechnoratiFurl this Post!
  #2 (permalink)  
Old 03-03-2003, 10:35 AM
mcaswell's Avatar
Caswell Inc Founder
 
Join Date: Nov 2001
Location: Lyons, NY USA
Posts: 2,374
Blog Entries: 2
mcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to beholdmcaswell is a splendid one to behold
Default

You might want to try freshening the zinc plate on your store bought parts with the plating kit, then chromating them.
__________________
--
Mike Caswell
Caswell Inc
http://www.caswellplating.com
Need Support? Visit our online support section at http://support.caswellplating.com
Have A Web Site?
Why not join our affiliate program and earn 15% of all sales. Join at http://www.caswellplating.com/affiliate.htm
Digg this Post!Add Post to del.icio.usBookmark Post in TechnoratiFurl this Post!
  #3 (permalink)  
Old 03-03-2003, 12:27 PM
Newbie
 
Join Date: Nov 2002
Posts: 27
aermakov@rogers.com
Default

That's what I did, will let you know when the parts dry out.
Digg this Post!Add Post to del.icio.usBookmark Post in TechnoratiFurl this Post!
  #4 (permalink)  
Old 03-03-2003, 07:28 PM
Newbie
 
Join Date: Mar 2003
Posts: 1
newman
Default

i too am having a hard time getting the yellow chromate to hold, right after i zinc plate i rinse with water and dunk into chromate for about 1-2 mins ,after 2-3 days i can remove all the color off with water and a rag, im running the bath @80%.... any ideas how to resolve this?
would a Nitric Dip help right before chromating?

thanks .

ps: im zinc plating old carb castings from the 60s.
Digg this Post!Add Post to del.icio.usBookmark Post in TechnoratiFurl this Post!
Closed Thread

Bookmarks


Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
 
Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off


Similar Threads
Thread Thread Starter Forum Replies Last Post
Copy Cad - Yellow Chromate does not stay on charlton Electroplating Questions 1 07-31-2005 12:52 PM
Chromate for Copy Cad/Zinc - Bright Blue kberger56 Caswell Please Sell This... 0 05-09-2005 12:32 AM
Copy Cad kit - blackener and yellow cad durability problems Broke Electroplating Questions 11 01-09-2005 11:19 AM
Yellow Chromate on Galvanized? Rickc Electroplating Questions 0 01-31-2004 06:19 PM
Copy Cad: Flat items okay; bolts dark? red911 Electroplating Questions 5 11-08-2003 09:17 PM


All times are GMT -4. The time now is 08:37 PM.


Powered by vBulletin® Version 3.8.4
Copyright ©2000 - 2009, Jelsoft Enterprises Ltd.
Search Engine Friendly URLs by vBSEO 3.3.0
Copyright © Caswell Inc.