This is a tool I machined and nickel plated.


Material: Brass rod stock.


Plating information:


Prep: Highly polished and pickled prior to going into nickel bath.
Voltage: 2.25Vdc
Current: 85ma. per square in.
Connector alignment tool
Pic Description: This is a tool I machined and nickel plated.


Material: Brass rod stock.


Plating information:


Prep: Highly polished and pickled prior to going into nickel bath.
Voltage: 2.25Vdc
Current: 85ma. per square in.
Agitation method: Large air bubbles and auto-rotation.
Hanger wire: .040" dia. oxygen free copper wire.
Anodes: Nickel 200, (2) 4"x6" on both sides of the 2-gallon tank.
Time: 1 hour
Plating thickness: .001"
Post buffing: None