Default Xtreme Chrome + Candy Gold?

I am planning on buying Xtreme Chrome and Candy Gold as a top color. Can anyone recommend finishing procedures? My friend who did the coating for my parts has the Hotcoat setup. Will it provide enough power to do this type of finish?
Reply With Quote
  #2 (permalink)  
Old 02-24-2007, 11:10 PM
baz baz is offline
Experienced Metal Finisher
 
Join Date: Feb 2006
Posts: 348
baz has a spectacular aura aboutbaz has a spectacular aura about
Default Re: Xtreme Chrome + Candy Gold?

Quote:
Originally Posted by UrineMachine
I am planning on buying Xtreme Chrome and Candy Gold as a top color. Can anyone recommend finishing procedures? My friend who did the coating for my parts has the Hotcoat setup. Will it provide enough power to do this type of finish?
candy gold over chrome plating looks nice . over polishing also but over extreme or near chrome it looks more like a butterscotch color not very nice i my opinion
Reply With Quote
  #3 (permalink)  
Old 02-25-2007, 12:01 PM
Amateur Metal Finisher
 
Join Date: Apr 2006
Posts: 78
UrineMachine is on a distinguished road
Default Re: Xtreme Chrome + Candy Gold?

Quote:
Originally Posted by baz
candy gold over chrome plating looks nice . over polishing also but over extreme or near chrome it looks more like a butterscotch color not very nice i my opinion

What is the best procedure for applying it? I will be doing it over xtreme chrome using an Eastwood kit. Any recommendations?
Reply With Quote
  #4 (permalink)  
Old 02-25-2007, 12:20 PM
Harleydad's Avatar
Metal Finishing Guru
 
Join Date: Dec 2006
Location: Wisconsin
Posts: 573
Harleydad is an unknown quantity at this point
Default Re: Xtreme Chrome + Candy Gold?

Quote:
Originally Posted by UrineMachine
What is the best procedure for applying it? I will be doing it over xtreme chrome using an Eastwood kit. Any recommendations?
Fully cure the xtreme. Some will let the part cool to room temp before the Candy Gold and some will shoot it at about 150 degrees, your choice (maybe a few test pieces are in order). If you can turn down the voltage for 2nd coats, do it. Make sure you have a good ground.
Reply With Quote
  #5 (permalink)  
Old 02-25-2007, 08:37 PM
Amateur Metal Finisher
 
Join Date: Apr 2006
Posts: 78
UrineMachine is on a distinguished road
Default Re: Xtreme Chrome + Candy Gold?

Quote:
Originally Posted by Harleydad
Fully cure the xtreme. Some will let the part cool to room temp before the Candy Gold and some will shoot it at about 150 degrees, your choice (maybe a few test pieces are in order). If you can turn down the voltage for 2nd coats, do it. Make sure you have a good ground.
Thanks very much. Also, maybe I am an idiot but I cannot find "clear coat" on Caswells site. Additionally I tried to order product but it said Transaction Failed. Hrmph.
Reply With Quote
Reply

Bookmarks


Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
 
Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off

Similar Threads
Thread Thread Starter Forum Replies Last Post
Gold Plating on Copy Chrome. ppaan Electroplating Questions 1 07-13-2006 11:00 AM
I need to strip chrome from aluminum? RedRiver Electroplating Questions 14 04-23-2006 08:38 PM
Chrome and Nickel Removal Question (long) bentley86 Electroplating Questions 5 03-19-2006 04:32 PM
Chrome / Candy Millermatic Powder Coating Questions 11 07-30-2004 09:34 AM
Chrome Plug 'N Plate over gold finish ntd Electroplating Questions 2 06-17-2003 11:04 PM


All times are GMT -4. The time now is 08:19 PM.


Powered by vBulletin® Version 3.7.3
Copyright ©2000 - 2008, Jelsoft Enterprises Ltd.
Search Engine Friendly URLs by vBSEO 3.2.0 RC4
Copyright © Caswell Inc.