Default 2nd coat is messed up?!?!?!

I did a frame for a guy and i decided i would spray a 2nd coat on after it had cooled because i had missed a few spots. So i pre-heated the frame and then coated and it came out looking like a satin finish that is grainy. What did i do wrong?
Reply With Quote
  #2 (permalink)  
Old 03-26-2007, 06:39 PM
Experienced Metal Finisher
 
Join Date: Apr 2004
Posts: 466
jtagger19 is on a distinguished road
Default Re: 2nd coat is messed up?!?!?!

more info will be help full
a couple things can cause that.
what color
temps (pre heat and cure)
time in the oven etc.

it happend to me a couple times with some solid tone colors and if the second coat is applied at over 150.
Reply With Quote
  #3 (permalink)  
Old 03-28-2007, 03:37 AM
speeddemonrodsteration's Avatar
Newbie
 
Join Date: May 2005
Location: great falls MT
Posts: 49
speeddemonrodsteration
Default Re: 2nd coat is messed up?!?!?!

Quote:
Originally Posted by jtagger19
it happend to me a couple times with some solid tone colors and if the second coat is applied at over 150.

Exactly- the metal is hot enough to melt the powder but not to let it flow out. Also if the second coat isn't thick enough (due to not enough power, poor lighting ect..) it will have a grainy finish.
__________________
Save the trees- burn Rubber!
};^)>
Reply With Quote
Reply

Bookmarks


Currently Active Users Viewing This Thread: 1 (0 members and 1 guests)
 
Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Trackbacks are Off
Pingbacks are Off
Refbacks are Off

Similar Threads
Thread Thread Starter Forum Replies Last Post
Extreme Chrome with Clear Coat How to... hvac36 Powder Coating Questions 47 02-06-2008 10:57 PM
Two Tone Powder Coat engineerscott Powder Coating Questions 5 03-27-2006 12:44 PM
Candy top coat cracked ricelake Powder Coating Questions 4 02-19-2005 07:04 AM
reason for clear coat? Jay87T Powder Coating Questions 14 03-20-2004 12:41 PM
Second coat after a few days tcjm Powder Coating Questions 1 03-20-2004 01:36 AM


All times are GMT -4. The time now is 06:04 PM.


Powered by vBulletin® Version 3.7.4
Copyright ©2000 - 2008, Jelsoft Enterprises Ltd.
Search Engine Friendly URLs by vBSEO 3.2.0
Copyright © Caswell Inc.