    DYES OPTIMUM Ph





    RED BORDEAUX 6



    YELLOW 4A 6

    BLUE 4 A 6


    VIOLET 3D 6


    BLACK HBL 5.5


    GREEN SCG 6.6


    GOLD S 6


    TURQUOISE 5.5


    OLIVE DRAB 7.5


    GOLDEN ORANGE 7


    GREY BL 5.5


    BROWN GL 6.5


    TEAL 5.5


    ELECTRIC BLUE 6


    COPPER BF 7


    FLOURESCENT PINK unk

    BRONZE 5.5



    DEEP RED 5.5


    FLOURESCENT YELLOW 6


    GREEN AEN 6


    VIOLET DS 6


    GREY NLN 5.5


    YELLOW 3GL 6


    BROWN BL 6.5


    FAST BLUE 5.5


    ORANGE 3A 6
    Last edited by mcaswell; 09-01-2005, 02:46 PM.
    --
    Mike Caswell
    Caswell Inc
    http://www.caswellplating.com
    Need Support? Visit our online support section at http://support.caswellplating.com

  • #2
    Re: Anodizing Dye pH

    I had to search around to find how to adjust the ph and I'd thought I'd save someone else the trouble and post a link to it. Enjoy.
    http://forum.caswellplating.com/show...6387#post16387
    Justin Martin, VP
    Blackcote
    RR1 Box 116
    Liverpool, PA 17045
    www.blackcote.com
    [email protected]

    Comment


    • #3
      Re: Anodizing Dye pH

      pH for fluro pink is 5.5-6 got it from tech support today

      john
      will only make the best no rubbish or can't sleep
      C/F TRIGGERS AVAILABLE NOW
      http://smg.photobucket.com/albums/v471/acidcustom/
      check out the link for parts available now
      http://smg.photobucket.com/albums/v471/acidcustom/
      [email protected]

      Comment


      • #4
        Re: Anodizing Dye pH

        I got a electronic PH tester. Do I put it into the black dye directly to measure the PH when the solution is cold or hot? I'm afraid the black dye is going to discolor the PH tester because it yellow plastic.

        Comment


        • #5
          Re: Anodizing Dye pH

          The plastic ph testers work well. Calibrate first. Cold Dye. Adding dye will usually raise the ph. Sometimes if ph is too high the dye won't absorb properly. We had problems with reds because of high ph in the past.
          Anodize World

          Comment


          • #6
            Hey guys,

            I was wondering if just "ph up" (Sodium Carbonate, Soda Ash) and "ph down" (Sodium Bisulfate) from a store would work for altering ph levels in the dyes? Or are acids necessary?

            Thanks!

            Comment


            • #7
              Hi Brwn253,
              To raise the PH, you will need to use Sodium Hydroxide, to lower the PH, use Acetic Acid.
              --
              Jason Vanderbroek
              315 946 1213 x116
              www.caswellplating.com

              Comment


              • #8
                Originally posted by Caswellplating_Jason View Post
                Hi Brwn253,
                To raise the PH, you will need to use Sodium Hydroxide, to lower the PH, use Acetic Acid.
                Hi Jason,

                Does the Acetic Acid need to be 99.85% can we get away with a Certified Food Grade - High Purity Ethanoic Acid at a lower grade ?
                https://www.ebay.co.uk/itm/500ml-Ace...d/131775286037

                Sodium Hydroxide With a purity of over 99.4% Supplied in micro prill form. be ok mixed with Distilled water ?
                https://www.ebay.co.uk/itm/750g-Sodi...c/143537134686


                Thanks

                Comment


                • #9
                  It doesn't matter where you get the acid or base from, nor does it matter what the initial concentration is. What matters is that 1) it doesn't have anything else in it (i.e. it's fairly pure), and 2) you know what concentration you are starting from so you can calculate the add quantity.

                  Even if you don't know #2, you can still make it work by making small adds and checking the bath pH after each add.
                  Process control doesn't give you good quality, it gives you consistent quality.
                  Good quality comes from consistently doing the right things.