    Can I chrome aluminum? It doesnt say what alloys I can chrome so I'm confused on this after attempting to chrome some small aluminum parts. Its the plug and plate kit.


    EDIT: upon searching the other plating kits I come across the other copy chrome kit and is says I need Zincate Primer for aluminum

  • #2
    You can't brush plate aluminum. You need to Zincate the part, then immersion plate with any of our plating baths.
    --
    Mike Caswell
    Caswell Inc
    http://www.caswellplating.com
    Need Support? Visit our online support section at http://support.caswellplating.com

    Comment


    • #3
      I just ordered some Zincate. Can I still use the Plug in Plate copy chrome kit, if I do the porper steps for emersing the part in a glass container with the wand clapmed to the glass while its emmeresed in the copy chrome solution? After I use the zincate on the aluminum parts.

      Comment


      • #4
        Yes, that will work.
        --
        Mike Caswell
        Caswell Inc
        http://www.caswellplating.com
        Need Support? Visit our online support section at http://support.caswellplating.com