    Is it necessary to dechrome chromed parts before silvering them? What is the best voltage and temperature for silver? Thanks alot, Gus
    I'm into modifying and inventing

  • #2
    Slver Plating

    I have one also: I purchased a Copy Chrome PlugNplate Kit and a bottle of Silver Solution. May I use the wand from the Chrome kit for silver plating or do I need a silver anode? What is the wand made of?
    I Rework Sax Mouthpieces. Some photos at www.mojomouthpiecework.com

    Comment


    • #3
      silver plating mouthpieces

      Mojo, A silver anode will preserve your silver solution. You could use an old silver fork or piece of sterling. Gus
      I'm into modifying and inventing

      Comment


      • #4
        Silver Plating

        Yes you need to de-chrome the silver first.

        Are you talking brush plating or tank plating? Tank plating requires 1.5-3 volts and 0.007 to 0.003 amps per square inch. 75 degress F works best.
        --
        Mike Caswell
        Caswell Inc
        http://www.caswellplating.com
        Need Support? Visit our online support section at http://support.caswellplating.com

        Comment


        • #5
          Silver Wand

          You can use the Copy Chrome Plug N Plate Wand to plate your silver. The wand is stainless steel.
          --
          Mike Caswell
          Caswell Inc
          http://www.caswellplating.com
          Need Support? Visit our online support section at http://support.caswellplating.com