    hi there laserman.

    Your lucky because polishing brake disk is my specialties.

    1- start with 240grit grinder
    2- then 320grit dual sander
    3- 600grit orbital 3/32"x 5"
    4- sisal + formax #37 compound
    5- treated airbuff + formax #34
    6- coton sewn 3/8"stitch + formax green
    7- flannel + formax blue

    Et voila (approx. 1 hour per disk both side)


    p.s. you also need a lot off patient because it's stainless 403 a very hard stainless to polish. if you need help write to me.
    good luck