  • ricelake
    replied
    candy coat cracked

    Originally posted by DALE
    Cracking in clearcoat can also come from the coating thickness being WAYYYYYYY to thick. This usually also comes with other defects as well.If you are only seeing cracking and nothing else then I agree with warchild.

    Hi Dale,Warchild was correct it was under cured.

    Leave a comment:


  • DALE
    replied
    Cracking in clearcoat can also come from the coating thickness being WAYYYYYYY to thick. This usually also comes with other defects as well.If you are only seeing cracking and nothing else then I agree with warchild.

    Leave a comment:


  • ricelake
    replied
    Cracked candy coat

    [quote="warchild"]This happen to me. The powder was under cured.[/
    quote]thanks warchild i ran a search for cracking and found your post from 2003.
    Thanks,Ken

    Leave a comment:


  • warchild
    replied
    This happen to me. The powder was under cured.

    Leave a comment:


  • ricelake
    started a topic Candy top coat cracked

    Candy top coat cracked

    Has anyone ever had a candy top coat get a bunch of cracks?I did a atv frame with a chrome base coat and flamboyant blue candy top coat.The whole frame is covered in little cracks.I've heard i might have baked the base coat to long,has anyone else been through this.