Re: scratches
Thanks for the info about the solvent test!
Announcement
Collapse
No announcement yet.
scratches
Collapse
X
-
Re: scratches
As Pickleboy stated, I've heard of a number of different methods for solvent tests. For poly's I used a 10% MEK/90% Xylene mix for 50 double rubs. No effect on the coating. After that I tried MEK alone. Usually only use that on epoxies but it didn't cut through the TGIC. It did soften the surface but if it wasn't cured I would have expected it to go down to the part or at least make a mess.
Think I will try Pickleboy's suggestion of waxing before any handling. I have waxed after the fact and it does help hide.
Anyone tried a different type of gloss black powder that resisted scratching but was still had good weathering properties?
Leave a comment:
-
Re: scratches
Originally posted by SheCoatsThanks for the comments and the welcome Pickleboy.
Manufactures data sheet calls for the 10 minutes @ 400F. Sprayed a few test panels today for DSC testing from powder manufacturer. Can't scratch the coating with a fingernail any more than with a towel. What about a clear coat over the black? Any potential delamination or clear discoloring issues to consider?
wamontgomery the solvent test is done after a full cure cycle to test the finish. on a full cooled part using a soft cloth and acetone or mek on the cloth rub the finished part in the same spot for about 30-50(opinions vary on this) strokes. if the powder is properly cured it will not color bleed on the cloth and will not fade. if it does it was not fully cured.
hope this helps.
Leave a comment:
-
Re: scratches
Originally posted by SheCoatsI'm using a high gloss TGIC black and noticing small micro scratches in the finish product.
Leave a comment:
-
Re: scratches
Can someone give me more detail about the solvent test?
Leave a comment:
-
Re: scratches
Thanks for the comments and the welcome Pickleboy.
Manufactures data sheet calls for the 10 minutes @ 400F. Sprayed a few test panels today for DSC testing from powder manufacturer. Can't scratch the coating with a fingernail any more than with a towel. What about a clear coat over the black? Any potential delamination or clear discoloring issues to consider?
Leave a comment:
-
Re: scratches
first off welcome to the forum.
from my experience black is prone to show scratches. also in addition to the solvent test you may want to do a scratch test with a fingernail in a inconspicuous place. if it scratches (indents) the powder, it is under cured. it should be able to withstand most temp ranges that will come in to play on most motorcycles, except exhaust temp. that requires high temp or ceramic coating. i have not yet, but others i know, have had good luck with standard powder, doing cylinders and heads as well as cases on cycle engines. lastly not to dispute the manufacture but all the powder i have used is at least 20 minutes cure cycle.
Leave a comment:
-
scratches
I'm using a high gloss TGIC black and noticing small micro scratches in the finish product. These scratches develope after wiping lint or dust off coated parts. Even if there is nothing on it you can take a soft towel and this will still leave scratches. Manufacture recommended cure cycle is 10 min. @ 400 degrees. I don't start the 10 min. cure cycle until the part reaches 400 degrees. Iv'e even doubled the cure time to 20 minutes and still get the same result. Solvent rub test has shown coating to be fully cured. I have heard that high gloss blacks are prone to these scratches. Is this true? With these being motorcycle parts, is there a diffirent type of powder that should be used? In some cases the powder must put up with high engine temps. Any comments welcome.Tags: None
Leave a comment: